Abstract:The bursting temperature and bursting rate of green pellets have important effects on pellet production. Taking fine-grained titanium concentrate as the research object, the influences of forming pressure, the amount of binder added, and the moisture content of green pellets on the bursting performance of green pellets are studied. The results show that when the moisture content of the green ball declines, the molding pressure mildly increases, the amount of binder goes up, and the bursting performance of the pellet get better; when the moisture content of the green ball is 7%, the molding pressure is 8 MPa, and the amount of binder is 0.30%, the bursting temperature of the green balls can reach more than 900 ℃, and the pellets do not burst, which meets the production process requirements.